EN AW-6005A T6 and EN AW-5083 H14/H24/H34 are about equally stiff. Their densities are about the same. Per unit mass they are about equally stiff (25.93 and 25.93 MJ/kg). Strength: f_o = 235 MPa for EN AW-5083 H14/H24/H34, f_o = 225 MPa for EN AW-6005A T6.
ratio = EN AW-6005A T6 / EN AW-5083 H14/H24/H34 · log scale
Property
EN AW-5083 H14/H24/H34
EN AW-6005A T6
Unit
Ratio
¼×1×4×
E Young's modulus
70
70
GPa
1×
G Shear modulus
27
27
GPa
1×
ν Poisson's ratio
0.3
0.3
–
1×
ρ Density
2700
2700
kg/m³
1×
α Coefficient of thermal expansion
23
23
10⁻⁶/K
1×
λ Thermal conductivity
110
—
W/(m·K)
—
σ_e Electrical conductivity
16
—
MS/m
—
f_u Tensile strength (R_m)
300
270
MPa
0.9×
f_o 0.2 % proof strength
235
225
MPa
0.957×
f_o,haz 0.2 % proof strength in the heat-affected zone
135
115
MPa
0.852×
f_u,haz Tensile strength in the heat-affected zone
270
165
MPa
0.611×
E/ρ Specific stiffness E/ρ · derived
25.93
25.93
MJ/kg
1×
c₀ Bar wave speed √(E/ρ) · derived
5092
5092
m/s
1×
f/ρ Specific strength f/ρ · derived
87.04
83.33
kJ/kg
0.957×
Values at the first thickness band or product form of each material (EN 1999-1-1 · t ≤ 5 mm · DT; EN 1999-1-1 · t ≤ 5 mm · EP/O, ER/B). A minimum and a characteristic value are not the same kind of number — read the ratio as a guide. Each material's page lists every band and every source.
COOKIES
We use a few cookies to see which pages engineers actually read and where they get stuck, and to tell whether our Google Search ads led to a sign-up or a purchase. No retargeting, nothing that follows you to other sites. They only start if you accept; reject and they stay off, and the site works exactly the same.