Aluminium · Aluminium extrusions · isotropic

EN AW-6082 T4

EN 1999-1-1 · extrusions and drawn tube · buckling class B

EN AW-6082 T4 is an aluminium alloy and temper for extrusions to EN 1999-1-1. Its characteristic 0.2 % proof strength is 110–110 MPa, depending on the product form and thickness. E = 70 GPa, ν = 0.3 and α = 23 × 10⁻⁶/K (design values).

Record
al-6082-t4-ext
Library
v1.1.0
Properties
11
Sources
2
Build check
passed ✓
Viewing as
guest
+ Compare Cite Download · PRO
E · Young's modulus 70GPa design[1]
ν · Poisson's ratio 0.3– design[1]
f_o · 0.2 % proof strength 110MPa char[1]EP, ET, ER/B · t ≤ 25 mm
f_u · Tensile strength (R_m) 205MPa char[1]EP, ET, ER/B · t ≤ 25 mm
ρ · Density 2700kg/m³ design[1]
α · Coefficient of thermal expansion 2310⁻⁶/K design[1]
λ · Thermal conductivity 170W/(m·K) typical[2]
σ_e · Electrical conductivity 24MS/m typical[2]

Elastic constants

isotropic
SymbolPropertyValueUnitBasisRef.
E Young's modulus ⓘ EN 1999-1-1 3.2.5 70 GPa design [1]
G Shear modulus 27 GPa design [1]
ν Poisson's ratio 0.3 – design [1]
K Bulk modulus K = E / 3(1 − 2ν) 58.33 GPa derived —
λ_L Lamé constant λ_L = Eν / (1 + ν)(1 − 2ν) 40.38 GPa derived —
c₀ Bar wave speed c₀ = √(E/ρ) 5092 m/s derived —

Physical, thermal and electrical

at 20 °C
SymbolPropertyValueUnitBasisRef.
α Coefficient of thermal expansion ⓘ for T < 100 °C 23 10⁻⁶/K design [1]
ρ Density 2700 kg/m³ design [1]
λ Thermal conductivity ⓘ lower end of the datasheet range, 20 °C 170 (170 – 220) W/(m·K) typical [2]
σ_e Electrical conductivity ⓘ lower end of the datasheet range, 20 °C 24 (24 – 32) MS/m typical [2]

Strength

a band applies up to and including its upper limit
PropertyProduct formThicknessValueUnitBasisRef.
f_oEP, ET, ER/B — EP, ET, ER/Bt ≤ 25 mm110MPachar[1]
f_uEP, ET, ER/B — EP, ET, ER/Bt ≤ 25 mm205MPachar[1]
SymbolPropertyValue at t = 25 mm · EP, ET, ER/BUnitBasisRef.
f_o 0.2 % proof strength ⓘ thickness is the upper limit of each row 110 MPa char [1]
f_u Tensile strength (R_m) 205 MPa char [1]
f_o,haz 0.2 % proof strength in the heat-affected zone ⓘ MIG welding; EN 1999-1-1 reduces HAZ values for TIG and thicker parts 100 MPa char [1]
f_u,haz Tensile strength in the heat-affected zone 160 MPa char [1]

Sources

every value names one
  1. EN 1999-1-1:2007, Eurocode 9 — Design of aluminium structures, Table 3.2b and 3.2.5Copies checked: 1, 2, 3, 4
  2. Wieland aluminium datasheets: EN AW-1050A, 5083, 6061, 6082Copies checked: 1, 2, 3, 4

min product standard minimum char characteristic design code value for design typical datasheet or textbook derived worked out here, formula shown

Cite this page

for reports and papers

BadgerMecX Materials (2026). EN AW-6082 T4 — material properties, EN 1999-1-1. Library v1.1.0, record al-6082-t4-ext. https://www.badgermecx.com/materials/al-6082-t4-ext/ (accessed 2026-11-26).

@misc{badgermecx_al6082t4ext,
  title  = {EN AW-6082 T4 -- material properties, EN 1999-1-1},
  author = {{BadgerMecX Materials}},
  year   = {2026},
  note   = {Library v1.1.0, record al-6082-t4-ext},
  url    = {https://www.badgermecx.com/materials/al-6082-t4-ext/}
}

Export and related