Timber · Solid timber, hardwood · orthotropic

D50

EN 338:2016 · strength class, 12 % moisture reference

D50 is a hardwood strength class to EN 338:2016. Its characteristic bending strength is 50 MPa. Along the fibres E₁ = 14 GPa; across them E₂ = 0.93 GPa.

Record
timber-d50
Library
v1.1.0
Properties
14
Sources
1
Build check
passed ✓
Viewing as
guest
+ Compare Cite Download · PRO
E₁ · Modulus, direction 1 14GPa mean[1]
f_m,k · Bending strength 50MPa char[1]
f_t,0,k · Tension parallel to grain 30MPa char[1]
ρ · Density 740kg/m³ mean[1]

Elastic constants

orthotropic
SymbolPropertyValueUnitBasisRef.
E₁ Modulus, direction 1 ⓘ E_0,mean, along the grain 14 GPa mean [1]
E₀,₀₅ Modulus parallel to grain, 5 % fractile 11.8 GPa char [1]
E₂ Modulus, direction 2 ⓘ E_90,mean, across the grain 0.93 GPa mean [1]
E₃ Modulus, direction 3 ⓘ E_90,mean — the standard does not separate radial and tangential 0.93 GPa mean [1]
G₁₂ Shear modulus 1-2 ⓘ G_mean 0.88 GPa mean [1]
G₁₃ Shear modulus 1-3 ⓘ G_mean 0.88 GPa mean [1]

Physical, thermal and electrical

at 20 °C
SymbolPropertyValueUnitBasisRef.
ρ Density 740 kg/m³ mean [1]
ρ_k Density, characteristic (5 % fractile) 620 kg/m³ char [1]

Strength

a band applies up to and including its upper limit
SymbolPropertyValueUnitBasisRef.
f_m,k Bending strength 50 MPa char [1]
f_t,0,k Tension parallel to grain 30 MPa char [1]
f_t,90,k Tension perpendicular to grain 0.6 MPa char [1]
f_c,0,k Compression parallel to grain 30 MPa char [1]
f_c,90,k Compression perpendicular to grain 6.2 MPa char [1]
f_v,k Shear strength 4.5 MPa char [1]

Notes

  • EN 338 and EN 14080 give no Poisson's ratios; a 3D analysis needs them from another source.

Sources

every value names one
  1. EN 338:2016, Structural timber — Strength classes, Tables 1 and 3Copies checked: 1, 2, 3

min product standard minimum char characteristic design code value for design typical datasheet or textbook derived worked out here, formula shown

Cite this page

for reports and papers

BadgerMecX Materials (2026). D50 — material properties, EN 338:2016. Library v1.1.0, record timber-d50. https://www.badgermecx.com/materials/timber-d50/ (accessed 2026-11-26).

@misc{badgermecx_timberd50,
  title  = {D50 -- material properties, EN 338:2016},
  author = {{BadgerMecX Materials}},
  year   = {2026},
  note   = {Library v1.1.0, record timber-d50},
  url    = {https://www.badgermecx.com/materials/timber-d50/}
}

Export and related

SI units, every value with basis and source