Timber · Glued laminated timber, combined · orthotropic

GL30c

EN 14080:2013 · strength class

GL30c is a combined glued laminated timber class to EN 14080:2013. Its characteristic bending strength is 30 MPa. Along the fibres E₁ = 13 GPa; across them E₂ = 0.3 GPa.

Record
glulam-gl30c
Library
v1.1.0
Properties
15
Sources
1
Build check
passed ✓
Viewing as
guest
+ Compare Cite Download · PRO
E₁ · Modulus, direction 1 13GPa mean[1]
f_m,k · Bending strength 30MPa char[1]
f_t,0,k · Tension parallel to grain 19.5MPa char[1]
ρ · Density 430kg/m³ mean[1]

Elastic constants

orthotropic
SymbolPropertyValueUnitBasisRef.
E₁ Modulus, direction 1 ⓘ E_0,g,mean 13 GPa mean [1]
E₀,₀₅ Modulus parallel to grain, 5 % fractile 10.8 GPa char [1]
E₂ Modulus, direction 2 ⓘ E_90,g,mean 0.3 GPa mean [1]
E₃ Modulus, direction 3 ⓘ E_90,g,mean 0.3 GPa mean [1]
G₁₂ Shear modulus 1-2 ⓘ G_g,mean 0.65 GPa mean [1]
G₁₃ Shear modulus 1-3 ⓘ G_g,mean 0.65 GPa mean [1]
G₀₅ Shear modulus, 5 % fractile 0.54 GPa char [1]

Physical, thermal and electrical

at 20 °C
SymbolPropertyValueUnitBasisRef.
ρ Density 430 kg/m³ mean [1]
ρ_k Density, characteristic (5 % fractile) 390 kg/m³ char [1]

Strength

a band applies up to and including its upper limit
SymbolPropertyValueUnitBasisRef.
f_m,k Bending strength 30 MPa char [1]
f_t,0,k Tension parallel to grain 19.5 MPa char [1]
f_t,90,k Tension perpendicular to grain 0.5 MPa char [1]
f_c,90,k Compression perpendicular to grain 2.5 MPa char [1]
f_v,k Shear strength 3.5 MPa char [1]
f_c,0,k Compression parallel to grain ⓘ two of the copies checked print 25.5 24.5 MPa char [1]

Notes

  • EN 338 and EN 14080 give no Poisson's ratios; a 3D analysis needs them from another source.

Sources

every value names one
  1. EN 14080:2013, Timber structures — Glued laminated timber, Tables 4 and 5Copies checked: 1, 2, 3, 4

min product standard minimum char characteristic design code value for design typical datasheet or textbook derived worked out here, formula shown

Cite this page

for reports and papers

BadgerMecX Materials (2026). GL30c — material properties, EN 14080:2013. Library v1.1.0, record glulam-gl30c. https://www.badgermecx.com/materials/glulam-gl30c/ (accessed 2026-11-26).

@misc{badgermecx_glulamgl30c,
  title  = {GL30c -- material properties, EN 14080:2013},
  author = {{BadgerMecX Materials}},
  year   = {2026},
  note   = {Library v1.1.0, record glulam-gl30c},
  url    = {https://www.badgermecx.com/materials/glulam-gl30c/}
}

Export and related

SI units, every value with basis and source